News

The Production Process Of Tungsten Rhenium Thermocouples

Feb 06, 2024 Leave a message

1: Preparation of Pre alloyed Powder

Weigh the components of the negative electrode material and positive electrode material according to weight percentage, prepare the negative electrode material and positive electrode material respectively, use high-energy dispersion method, reverse three speed 80-150r/min, dispersion time 15-20h

2: Forming

Mechanical compression molding, pressure 150-450Mpa, time 15-20s

3: Pre sintering

Under a reducing atmosphere of 1300-1500 ° * 3h

4: Vertical fusion

Divided into two sections, the first section is 2000A * 20min, and the second section is 2800-3300A * 450min

5: Rotary forging:

Temperature 1300-1600 ° C, pass compression rate greater than 25%, machining size range 10% -20%

6: Cleaning

Alkali electrolysis cleaning, alkaline concentration: 15-20%, electrolysis voltage 30-100V, time 5 seconds

7: Annealing

Finished wire annealing temperature 1200-1500 ° C, time 30-60 minutes

8: Finished product packaging

Vacuum packaging

Send Inquiry